22, Some part with white/milky color on the bottle surface after blowing
A, Causes:
   1, Heating temperature for the white color part is too high
   2, Stretch ratio is too big
   3, Water inside the compressed air

B, Solutions:
   1, Reduce the heating temperature for the white color part on the heating oven
   2, Get good quality preforms
   3, Make the stretch rod to a little slower
   4, replace the oil filter

23, PET bottle is not strong enough
A, Causes:
   1, Thickness of the bottles are not even
   2, Heating temperature is too high for the whole body
   3, Bottle design is not good

B, Solutions:
   1, Fix the injection molds for the PET preforms
   2, Get good quality preforms
   3, Fix the heating tunnel, make sure all heating lamps are in the right position
   4, Reduce the heating temperature for the thickness-not-even part
   5, Increase the molds air extraction
   6, Better to make the bottle by low temperature and high compressor
   7, Re-design the bottles

http://www.sinobema.com/Difference-between-bottles-of-pure-water?article_id=199
From Sino Beverage Machinery Co., Ltd China
施诺机械设备有限公司中国
sinobema@gmail.com
www.sinobema.com 

www.sinobeveragemachinery.com
WhatsApp: 0086 137 28668423



没有评论:

发表评论

Bottling filling machinery.

Different machines/models for differnet bottles. Email: sinobema@gmail.com WhatsApp: 0086 137 2866 8423 www.sinobema.com Sino Beverage M...